| Common Names: |
|
American ash
Ash
Biltmore ash
Biltmore white ash
Fresno
White ash
|
|
|
|
|
|
- Mechanical Values
| Category |
Green |
Dry |
Units |
| Weight |
51 |
43 |
lbs/cu.ft. |
| Density (air-dry) |
|
|
lbs/cu.ft. |
| Specific Gravity |
0.56 |
0.67 |
|
| Hardness |
|
1320 |
lbs |
| Stiffness |
1435 |
1720 |
1000 psi |
| Bending Strength |
8900 |
15050 |
psi |
| Shearing Strength |
|
1910 |
psi |
| Max. Crushing Strength |
3905 |
7420 |
psi |
| Work to Maximum Load |
20 |
20 |
in-lbs/in3 |
| Radial Shrinkage (G->OD) |
|
5 |
% |
| Tangential Shrink. (G->OD) |
|
8 |
% |
| Volumetric Shrink (G->OD) |
|
13 |
% |
Environmental Profile
White ash is reported to be demonstrably widespread, abundant, and secure globally, although it may be quite rare at the periphery of its range (Source - The Nature Conservancy - Rank of relative endangerment based primarily on the number of occurrences of the species globally).
Distribution
The North American range of White ash is reported to include New Brunswick, Nova Scotia, Ontario, Prince Edward Island, Quebec, Alabama, Arkansas, Colorado, Connecticut, Delaware, Florida, Georgia, Indiana, Kansas, Kentucky, Louisiana, Massachusetts, Maryland, Maine, Michigan, Minnesota, Missouri, Mississippi, North Carolina, Great Smoky Mountain National Park, Iowa, Illinois, Nebraska, New Hampshire, New Jersey, New York, Ohio, Oklahoma, Pennsylvania, Rhode Island, South Carolina, Tennessee, Texas, Virginia, Vermont, Wisconsin, and West Virginia. The tree prefers moist soils of valleys and slopes, particularly deep, well-drained loams. It is usually found growing with many other hardwoods.
Product Sources
Some material from this species is reported to be available from sustainably managed, salvaged, recycled, or other environmentally responsible sources.
Supplies of Ash are reported to be plentiful on the US market. The cost of Ash, which was once moderate, is reported to be steadily rising.
The following species in the database have been suggested as potential substitutes for ash:
African celtis (Celtis mildbraedii )
Axlewood (Anogeissus latifolia )
White tabebuia (Tabebuia insignis )
The following species in the database is also reported to have similar properties to ash:
Santa maria (Calophyllum brasiliense )
Indicated strength properties of the following species in the database are reported to be similar to those of White ash:
Silver birch (Betula pendula ) Toughness
Brown sterculia (Sterculia rhinopetala ) Toughnesss
Australian blackwood (Acacia melanoxylon ) Impact
Tree Data
White ash is reported to be the largest and most important of the 18 Ash species that are native to the United States. Trees often attain heights of 70 to 80 feet (21 to 24 m), with trunk diameters of 24 to 36 inches (60 to 90 cm). Boles are are reported to be often straight and clear of branches to 30 to 50 feet (9 to 15 m).
Sapwood Color
The narrow sapwood is nearly white in color.
Heartwood Color
The heartwood is pale brown, grayish brown, light brown, or pale yellow streaked with brown. The color may also be cream to very light brown, occasionally with a reddish tinge.
Grain
The grain is described as bold, straight, moderately open with an occasional wavy pattern. Plainsawn boards usually have strong contrast in grain.
Texture
The material is normally coarse-textured.
Luster
The wood is reported to be lustrous.
Odor
Ash is reported to be typically free from taste and odor.
Ease of Drying
Air-seasoning is reported to occur at a faster rate than average, with very little shrinkage. Kiln-drying yields satisfactory results, but low initial temperates are required.
Drying Defects
Drying degrade common in this species include gray-brown sapwood stains (sticker marks, stains), and surface checks (in 6/4 and thicker stock). These are attributable to trees from wet sites, drying too slowly. Distortion and end-splitting may also occur, and existing shakes may open up.
Kiln Schedules
T8-B4 (4/4), T5-B3 (8/4) US
Movement in Service
White ash is reported to have good dimensional stability, and is superior to Red oak in this property.
T/R Ratio
1.63
This indicator is more meaningful if it is used together with other drying information and actual shrinkage data in the tangential and radial directions. (Refer to the Numerical Values window).
Natural Durability
The heartwood is reported to have little or no natural resistance to attack by decay causing organisms and insects. The sapwood is also susceptible to attack by powder post beetle and fungi.
Resistance to Impregnation
The wood is reported to respond well to preservative treatment.
Veneering Qualities
Ash is used to manufacture plywood and some logs are sliced into decorative veneers for paneling and furniture uses.
Cutting Resistance
There is very little cutting resistance.
Blunting Effect
There is moderate blunting effect on cutting tools.
Planing
The wood is fairly easy to plane.
Turning
Turning properties are reported to be rather poor.
Boring
The wood is characteristically very easy to bore.
Mortising
Mortising properties are reported to be poor.
Gluing
Under controlled conditions, Ash is reported to glue with satisfactory results.
Nailing
White ash is reported to possess good resistance to splitting, and has good nail-holding properties.
Screwing
The timber has fairly good screwing properties.
Sanding
The wood is reported to have satisfactory sanding characteristics.
Polishing
Polishing qualities are reported to be good.
Staining
The wood has good staining characteristics and is often finished in black.
Varnishing
The wood has satisfactory varnishing qualities.
Painting
Painting properties are reported to be satisfactory.
Steam Bending
The wood has satisfactory or fairly good steam bending characteristics.
Response to Hand Tools
The wood works well with hand tools.
|